产品中心/ISO 4954
MATERIAL DATA · COLD FORMING
22MnB4 冷镦钢丝
22MnB4 冷镦钢丝技术资料,执行标准为 ISO 4954。查看当前牌号的化学成分、力学性能及相关技术要求。
22MnB4 · 冷镦钢丝
01执行标准ISO 4954
02材料牌号22MnB4
03材料形态冷镦钢丝
04交货说明按订单技术条件确认
STANDARD & PROPERTIES
材料技术参数
1.交货条件的组合
表B.1-交货时热处理条件、产品形式和适用要求的组合
| Heat-treatment condition at delivery | Symbol | Products form a | Applicable requirements in cases where the steel concerned has been ordered with reference to the steel names indicated in |
|---|
| Wire rod | Bar | Wire | T a b les B. 2,B.3,B.4 or B.5 | Ta bles B. 2,B.3,B.4,B.5,B.6 or B,7 | Optional |
| As hot-rolled or peeled | +AR or +PE | X | X | X | Chemical composition as specified in Table B.2 | Mechanical properties as specified in Ta b le s B.3 ,B.4 and B.5 | Chemical compositior as specified in Table B.2 | Mechanical properties as specified in Tables B,3, B.4 and B.5 | Values for hardenability according to Ta ble s B.6 and B.7 | Supplementa- ry or special requirements as specified in Annex Eh |
| Cold drawn | +AR+C | - | X | X |
| Cold drawn + spheroidized | +AR+C+AC | - | X | X |
| Cold drawn + spheroidized+skin passed | +AR+C+AC +LC | - | X | X |
| Spheroidized or spheroidized+peeled | +AC or +AC +PE | X | X | X |
| Spheroidized+cold drawn | +AC+C | | X | X |
| Treated to ferrite- pearlite structure and hardness range | +FP | - | X | - |
| Others | Other delivery conditions may be agreed at the time of ordering |
| a X=applicable,-=not applicable. b If agreed at the time of the enquiry and order. |
2.化学组成
表B.2-表面硬化用钢的化学成分 (适用于铸造分析)
3.力学性能
表B.4-硼合金钢牌号的力学性能
| Steel name | Diameter | Delivery condition |
|---|
| +AR | +AC or +AC+PE | +AR+C | +AR+C+AC | +AR+C+AC+LC | +AC+C |
| above mm | up to mm | Rm max. MPa | Za min % | Rm max. MPa | Z min. % | Rm max. MPa | Z min % | Rm max. MPa | Z min. % | Rm max. MPa | Z min. % | Rm max. MPa | Z min. % |
| 22MnB4 | 2 | 5 | | — | — | | | | 520 | 64 | 560 | 62 | | — |
| 5 | 10 | 600 | 55 | 520 | 62 | 720 | 53 | 500 | 64 | 540 | 62 | 630 | 59 |
| 10 | 40 | 600 | 55 | 520 | 62 | 710 | 53 | 500 | 64 | 540 | 62 | 620 | 59 |
| a The values are given only for information. |
4.淬透性要求
表B.6-标准淬透性钢种的硬度限值 (H级)
| Steel name | Symbol | Austenitizing temperature ℃±5℃ | Limits of range | Hardness HRC at a distance from quenched end of test piece(in mm)of |
|---|
| 1,5 | 3 | 5 | 7 | 9 | 11 | 13 | 15 | 20 | 25 | 30 | 35 | 40 |
| 22MnB4 | +H | 880 | max. | 49 | 48 | 47 | 45 | 42 | 39 | 35 | 32 | 24 | 20 | | — | |
| min. | 43 | 41 | 40 | 32 | 23 | | | — | — | — | | — | |
化学成分、力学性能、交货状态及其他技术要求应以现行有效标准、客户图纸和订单技术协议为准;网页资料不替代正式质量证明文件。